TR0636E-20027 HIROSE
Document overview
- PDF pages: 6
Technical content
Page 1
1/6
TR0636E-20027
IT3D(M)-300S-BGA (57) BGA Shearing Force
TEST REPORT
| APPROVED | TY. ARAI |
| CHECKED | TM.MATSUO |
| PREPARED | TY.TAKADA |
HIROSE ELECTRIC CO., LTD.
Page 2
2/6
[1] Objective
To evaluate BGA shearing force by comparing Initial state and Post 3500 thermal cycle in accordance with IPC-9701.
[2] Specimens
| Type | Product | Assembly | State | # of specimens |
|---|---|---|---|---|
| Type_1 | IT3D-300S-BGA (57) | Virgin | Initial | 3 |
| Type_2 | IT3D-300S-BGA (57) | Reworked | Initial | 3 |
| Type_3 | IT3D-300S-BGA (57) | Virgin | Post 3500 cycles | 3 |
| Type_4 | IT3D-300S-BGA (57) | Reworked | Post 3500 cycles | 3 |

Remarks \*Type_3, Type_4 are assembled as Fig.1. \*The test board design is based on IPC-9701 specification. \*Thickness of the PCB: 3.3mm
Fig.1 [3] Test period
From: 2007-09-12 To : 2008-01-18
[4] Test Equipment
| Test equipment | Model | Manufacture |
| Insertion and withdrawal force tester | AG-IS | Shimazu |
Page 3
3/6
BGA shearing force
1. Requirements
The failure mode for the sheared balls shall be either bulk solder failure or copper pad lift-off. Intermetallic failure is unacceptable.
2. Conditions
2-1 Test Condition

2-2 BGA Shearing Force
IT3D-300S-BGA(57)
Insertion and withdrawal force tester

CONNECTOR Sample
0.3mm space
Test PCB
Page 4
4/6
- Results
4-1 BGA Shearing Force
UNIT: KN

4-2 Failure Mode
No intermetallic failure was found in all specimens. Copper pad lift-off was found in the sheared area.
Details are shown in the following pages.
Page 5
5/6
Type-1 (Initial) Virgin



Copper Pad lift-off
Type-2 (Initial) Reworked



Copper Pad lift-off
Page 6
6/6
Type-3 (Post 3500 thermal cycles) Virgin



Copper Pad lift-off
Type-4 (Post 3500 thermal cycles) Reworked



Copper Pad lift-off